In this Letter, we present the first direct loss tangent measurement of high resistivity (100) silicon wafers in the temperature range ~70 mK to 1 K. The measurement was performed by means of an innovative resonant technique taking advantage of a high quality factor superconducting niobium resonator, that allows to achieve unprecedented level of accuracy. We report Si loss tangent values at the lowest temperature one order of magnitude larger than what typically expected, and we observe non-monotonic trend of the loss tangent as a function of temperature. With this study, we established a new capability to directly measure the loss tangent of insulating materials with high accuracy and precision. This technique will allow to identify substrates and materials with low losses aiming to maximize coherence in quantum devices.
In this Letter, we present the first direct loss tangent measurement of high resistivity (100) silicon wafers in the temperature range ~70 mK to 1 K. The measurement was performed by means of an innovative resonant technique taking advantage of a high quality factor superconducting niobium resonator, that allows to achieve unprecedented level of accuracy. We report Si loss tangent values at the lowest temperature one order of magnitude larger than what typically expected, and we observe non-monotonic trend of the loss tangent as a function of temperature. With this study, we established a new capability to directly measure the loss tangent of insulating materials with high accuracy and precision. This technique will allow to identify substrates and materials with low losses aiming to maximize coherence in quantum devices.
In this letter, we present the direct loss tangent measurement of a high-resistivity intrinsic (100) silicon wafer in the temperature range from ~ 70 mK to 1 K, approaching the quantum regime. The measurement was performed using a technique that takes advantage of a high quality factor superconducting niobium resonator and allows to directly measure the loss tangent of insulating materials with high level of accuracy and precision. We report silicon loss tangent values at the lowest temperature and for electric field amplitudes comparable to those found in planar transmon devices one order of magnitude larger than what was previously estimated. In addition, we discover a non-monotonic trend of the loss tangent as a function of temperature that we describe by means of a phenomenological model based on variable range hopping conduction between localized states around the Fermi energy. We also observe that the dissipation increases as a function of the electric field and that this behavior can be qualitatively described by the variable range hopping conduction mechanism as well. This study lays the foundations for a novel approach to investigate the loss mechanisms and accurately estimate the loss tangent in insulating materials in the quantum regime, leading to a better understanding of coherence in quantum devices.
Superconducting resonators are central to superconducting quantum information technologies and essential for bosonic qubit architectures, where long-lived storage modes enable hardware-efficient error correction. Achieving ultra-high quality factors in scalable planar circuits is challenging because multiple dissipation channels contribute to the total loss. Here we report planar α-Ta resonators fabricated on 300 mm ultra-high-resistivity (>10 kΩ cm) intrinsic silicon using industrial processes, achieving median internal Q factors exceeding 40 million and maxima above 60 million. Energy-participation-ratio analysis identifies a dominant participation-controlled interface loss mechanism and places conservative upper bounds on substrate-associated dissipation. For the best-performing substrate, the inferred substrate loss tangent is below 1.0×10−8, establishing industrial MCZ silicon among the lowest-loss substrate platforms reported for superconducting resonators. At the same time, the exceptionally low losses show no clear correlation with commonly cited silicon substrate metrics such as room-temperature resistivity or impurity concentrations. More broadly, these studies establish industrial 300 mm processing, careful interface engineering, and 300 mm MCZ silicon substrates as a promising platform for resonator-heavy superconducting quantum architectures with ultra-high quality factors.
Understanding the correlation between material properties and microwave losses in superconducting films is a crucial subject for developing low-loss materials for quantum circuits. We focus on vanadium (V) as a novel material for superconducting quantum devices and discuss loss in V films in relation to their structural properties. Using a sputtering method, we grow four V-film structures on (001)-oriented Si wafers, employing Nb and Ta as the buffer and capping layer materials, respectively: Nb/V/Ta, Nb/V, V/Ta, and V. X-ray diffraction and atomic force microscopy reveal that the V films grown on the Nb buffer layers have higher uniformity of lattice orientation and smaller grain size than that directly grown on the Si wafer. Coplanar waveguide resonators are fabricated from the four V-film structures, and averaged photon number (⟨nph⟩) dependences of internal quality factor (Qint) are obtained by performing microwave measurements. By analyzing the obtained Qint vs ⟨nph⟩, it is found that loss at the V surface is dominated by ⟨nph⟩-independent non-two-level-system (non-TLS) losses, which can be mitigated by introducing the Ta capping layer. Furthermore, the V films on the Nb buffer layers exhibit lower Qint in the ⟨nph⟩ range from 100 to 106 and higher non-TLS loss than that directly grown on Si wafers, even though the former has higher lattice-orientation uniformity than the latter. Origins of these trends might be relevant to V oxides, of which presence at surfaces and grain boundaries in bulk regions in the V resonators is suggested by energy dispersive X-ray spectroscopy and X-ray photoelectron spectroscopy, and/or V hydrides.
Even though silicon is widely used in superconducting quantum processors as the substrate upon which qubits are fabricated, the effect of silicon on the performance of the qubits is not fully understood. Using ultrahigh-quality microwave cavities to measure dielectric loss with parts-per-billion precision, the authors clearly show that using silicon is detrimental to qubit coherence time. The loss tangent found here is an order of magnitude worse than previously measured. This study sheds light on the physical mechanisms behind dissipation in silicon, and highlights the need for further work to fully understand the origin of these losses, and how to mitigate them.
The improvement of the coherence times of superconducting qubits depends on the reduction of the dielectric losses in the insulating materials implemented for the device fabrication. These losses depend on the density of spurious dipoles of different nature (two-level systems, TLSs) which couple to phase qubits and, hence, limit their coherence times. Hydrogenated amorphous silicon (a-Si:H), because of its lower loss tangent (tan δ) among conventional dielectrics (a-SiO, a-SiO2, a-SiNx:H), is considered as the best amorphous dielectric for superconducting qubit application. We have developed a reliable method for the direct measurement of dielectric losses in amorphous dielectric thin films using a novel design based on four lumped superconducting LC resonators connected in series without coupling capacitors. The losses are obtained as tan δ = 1/Q0, where Q0 is the intrinsic quality factor of the resonator, measured at 3 dB above the resonance frequency without any fitting procedure. The series type LC resonators with a-Si:H as dielectric were fabricated by the Nb technology. The measurements were done at the conditions of a qubit application (0.5 -10 GHz frequency range and low temperatures). The low values of the loss tangent of a-Si:H (up to 2.5 x 10−5 at 4.2 K) have required the development of superconducting housing for the resonators in order to eliminate a spurious dependence of tan δ on the microwave power, by reducing losses which were not originated in the dielectric itself. The results of the simulations agree well with the experiments.
Low-loss dielectric films are an important component of superconducting circuits with applications ranging from quantum information to superconducting detectors for astrophysics. In millimeter-wave detector circuits, dielectric loss can be the limiting factor on efficiency and resonator performance. Some advantageous detector fabrication architectures require dielectric deposition at temperatures substantially lower than those conventionally used to achieve low dielectric loss. In this work, we characterize silicon nitride (SiNx) films deposited by inductively coupled plasma chemical vapor deposition (ICPCVD) at 150∘C for use in temperature-constrained superconducting detector fabrication. We measure the dielectric loss tangent of these films at ∼4−7 GHz using superconducting niobium microstrip resonators and extract the loss by fitting the temperature-dependent resonant frequency to a two-level-system model. We vary the N2/SiH4 precursor-flow ratio between dielectric depositions and find a clear trend of decreasing loss with decreasing N2/SiH4. We additionally find that applying an RF substrate bias during deposition reduces the loss compared to films deposited without bias. These results identify precursor ratio and substrate bias as practical process parameters for improving low-temperature SiNx for superconducting detector circuits.