The improvement of the coherence times of superconducting qubits depends on the reduction of the dielectric losses in the insulating materials implemented for the device fabrication. These losses depend on the density of spurious dipoles of different nature (two-level systems, TLSs) which couple to phase qubits and, hence, limit their coherence times. Hydrogenated amorphous silicon (a-Si:H), because of its lower loss tangent (tan δ) among conventional dielectrics (a-SiO, a-SiO2, a-SiNx:H), is considered as the best amorphous dielectric for superconducting qubit application. We have developed a reliable method for the direct measurement of dielectric losses in amorphous dielectric thin films using a novel design based on four lumped superconducting LC resonators connected in series without coupling capacitors. The losses are obtained as tan δ = 1/Q0, where Q0 is the intrinsic quality factor of the resonator, measured at 3 dB above the resonance frequency without any fitting procedure. The series type LC resonators with a-Si:H as dielectric were fabricated by the Nb technology. The measurements were done at the conditions of a qubit application (0.5 -10 GHz frequency range and low temperatures). The low values of the loss tangent of a-Si:H (up to 2.5 x 10−5 at 4.2 K) have required the development of superconducting housing for the resonators in order to eliminate a spurious dependence of tan δ on the microwave power, by reducing losses which were not originated in the dielectric itself. The results of the simulations agree well with the experiments.
Low-loss deposited dielectrics will benefit superconducting devices such as integrated superconducting spectrometers, superconducting qubits, and kinetic inductance parametric amplifiers. Compared with planar structures, multilayer structures such as microstrips are more compact and eliminate radiation loss at high frequencies. Multilayer structures are most easily fabricated with deposited dielectrics, which typically exhibit higher dielectric loss than crystalline dielectrics. We measure the subkelvin and low-power microwave and millimeter-submillimeter-wave dielectric loss of hydrogenated amorphous silicon carbide (
a-SiC:H), using superconducting chips with Nb-Ti-
N/a-SiC:H/Nb-Ti-N microstrip resonators. We deposit the
a-SiC:H by plasma-enhanced chemical vapor deposition at a substrate temperature of $400{\phantom{\rule{0.1em}{0ex}}}^{\ensuremath{\circ}}\mathrm{C}$. The
a-SiC:H has a millimeter-submillimeter loss tangent ranging from $0.9\ifmmode\times\else\texttimes\fi{}{10}^{\ensuremath{-}4}$ at 270 GHz to $1.5\ifmmode\times\else\texttimes\fi{}{10}^{\ensuremath{-}4}$ at 385 GHz. The microwave loss tangent is $3.1\ifmmode\times\else\texttimes\fi{}{10}^{\ensuremath{-}5}$. These are the lowest low-power subkelvin loss tangents that have been reported for microstrip resonators at millimeter-submillimeter and microwave frequencies. The
a-SiC:H films are free of blisters and have low stress: $\ensuremath{-}20$ MPa compressive at 200-nm thickness to 60 MPa tensile at 1000-nm thickness.