Nitrogen-vacancy centers in diamond are promising as sensitive vector magnetometers, quantum repeaters, and qubits, but realizing this potential has been limited by the diamond material itself. Here a comprehensive study addresses creation of nitrogen-vacancy centers, balancing the impact of irradiation and annealing on the quantum coherence properties of commercial material. Photoluminescence decomposition analysis is used to quantitatively determine the neutral-to-negative charge-state ratio, and for insight into the impact of electron irradiation on material quantum coherence properties.
Nitrogen-vacancy centers in diamond are promising as sensitive vector magnetometers, quantum repeaters, and qubits, but realizing this potential has been limited by the diamond material itself. Here a comprehensive study addresses creation of nitrogen-vacancy centers, balancing the impact of irradiation and annealing on the quantum coherence properties of commercial material. Photoluminescence decomposition analysis is used to quantitatively determine the neutral-to-negative charge-state ratio, and for insight into the impact of electron irradiation on material quantum coherence properties.
The negatively charged nitrogen-vacancy (NV-) center in diamond is a promising spin system for quantum sensing applications. NV-ensembles are favored for an improved signal-to-noise ratio and sensitivity. The optimization of diamond with NV-ensembles often requires a high NV concentration, a long spin coherence time T2 and a stable charge state. However, these key requirements are interdependent and can be difficult to optimize: nitrogen impurities as the main decoherence source of the NV spin limits the coherence time T2, and pursuing high NV concentration can deteriorate the NV-charge-state stability. Consequently, their best achievable combination becomes an essential question for the material characterization. In this work, we systematically investigate the NV center creation and properties in chemical vapor deposition (CVD) diamond. We have grown CVD diamond series with a varying nitrogen flow over four orders of magnitude, leading to a broad range of single substitutional nitrogen (P1 center) densities from 0.2 to 20 ppm. On these series, we study P1, NV creations and NV charge states after growth, as well as their transformation under subsequent electron beam irradiation. Furthermore, for a fixed nitrogen concentration, we optimize electron-irradiation fluences with two different accelerated electron energies. We discuss a general approach to determine the optimal irradiation conditions, for which an enhanced NV concentration and an optimum of NV charge states can both be satisfied. Moreover, through irradiation and annealing treatments, we monitor the change in T2 and aim to increase the NV density without compromising T2. We achieve NV concentrations from 1 to 168 ppb with T2 from 549 to 45.5 µs respectively. This study shows a pathway to engineer properties of NV-doped CVD diamonds for improved sensitivity.
Abstract The nitrogen-vacancy (NV) center in diamond is a promising quantum system for magnetometry applications exhibiting optical readout of minute energy shifts in its spin sub-levels. Key material requirements for NV ensembles are a high NV − concentration, a long spin coherence time and a stable charge state. However, these are interdependent and can be difficult to optimize during diamond growth and subsequent NV creation. In this work, we systematically investigate the NV center formation and properties in bulk chemical vapor deposition (CVD) diamond. The nitrogen flow during growth is varied by over four orders of magnitude, resulting in a broad range of single substitutional nitrogen concentrations of 0.2–20 parts per million. For a fixed nitrogen concentration, we optimize electron-irradiation fluences with two different accelerated electron energies, and we study defect formation via optical characterizations. We discuss a general approach to determine the optimal irradiation conditions, for which an enhanced NV concentration and an optimum of NV charge states can both be satisfied. We achieve spin–spin coherence times T 2 ranging from 45.5 to 549 μ s for CVD diamonds containing 168 to 1 parts per billion NV − centers, respectively. This study shows a pathway to engineer properties of NV-doped CVD diamonds for improved sensitivity.
We created dense ensembles of negatively charged nitrogen-vacancy (NV-) centers in diamond by neutron and electron irradiation for applications in hybrid quantum systems and magnetometry. We characterize fluorescence intensity, optical and coherence properties of the resulting defects by confocal microscopy, UV/Vis and FTIR spectroscopy, optically detected magnetic resonance and small angle X-ray scattering. We find the highest densities of NV- at neutron fluences on the order of 10^17 cm^-2 and electron doses of 10^18 cm^-2, with spin resonance linewidths of 6 MHz. Lower electron energies increase the ratio of centers in the desired negative charge state to those in the neutral one. Annealing at 900 °C during the irradiation reduces the spin resonance linewidth. Electron irradiation furthermore results in substantially higher optical transparency compared to neutron irradiation.
Nitrogen-vacancy (NV) centers in single-crystal CVD diamond are promising candidates for quantum sensing due to their remarkable optical and spin properties [1]. These defects exhibit stable photoluminescence (PL), long spin coherence times, and high sensitivity to external fields [2]. In this study, we present a room-temperature PL characterization of NV centers excited with a 532 nm laser. The setup was optimized for high signal-to-noise ratio and spectral resolution. Key parameters analyzed include emission intensity, zero-phonon line (ZPL) at ~637 nm, phonon sidebands, and the charge state distribution between NV⁰ and NV⁻. The NV⁻ state, crucial for spin-based sensing, is evaluated to understand its stability under different nitrogen doping conditions [3]. The relative intensities of NV⁰ and NV⁻ provide insights into nitrogen incorporation and vacancy formation. These results contribute to optimizing synthesis conditions for enhanced NV⁻ concentration, supporting the advancement of diamond-based quantum sensing technologies.
Nitrogen vacancy (NV) centers in diamond are at the heart of many emerging quantum technologies, all of which require control over the NV charge state. Hence, methods for quantification of the relative photoluminescence intensities of the NV0 and NV− charge states, i.e., a charge state ratio, are vital. Several approaches to quantify NV charge state ratios have been reported but are either limited to bulk-like NV diamond samples or yield qualitative results. We propose an NV charge state quantification protocol based on the determination of sample- and experimental setup-specific NV0 and NV− reference spectra. The approach employs blue (400–470 nm) and green (480–570 nm) excitation to infer pure NV0 and NV− spectra, which are then used to quantify NV charge state ratios in subsequent experiments via least squares fitting. We test our dual excitation protocol (DEP) for a bulk diamond NV sample and 20 and 100 nm nanodiamond particles and compare results with those obtained via other commonly used techniques such as zero-phonon line fitting and non-negative matrix factorization. We find that DEP can be employed across different samples and experimental setups and yields consistent and quantitative results for NV charge state ratios that are in agreement with our understanding of NV photophysics. By providing robust NV charge state quantification across sample types and measurement platforms, DEP will support the development of NV-based quantum technologies.
Electron irradiation is one of the most powerful methods to create negatively charged nitrogen-vacancy centers (NV-s) in diamonds, which act as qubits and quantum sensors even at room temperature (RT). For quantum sensing, it is important to create ensemble NV-s with long coherence time (T2) since the sensitivity can be affected by both amount of NV- and T2. For high concentration NV-, electron irradiation with higher fluence is needed. However, if electron fluence is too high, neutral NVs (NV0s) are created because of lack of N donors. For T2, since residual defects act as origins of T2 decoherence, it is important to optimize the condition of subsequent annealing as well as irradiation fluence. Thus, we need to consider initial nitrogen (P1) concentration in diamond, electron fluence, and annealing conditions. In this paper, we create NV-s in Ib diamonds by electron irradiation and subsequent annealing with different conditions, and study the amounts of NV-s and their T2 for high-sensitive quantum sensing. The samples used in this study were Ib diamond with P1 concentration around 100 ppm. Those samples were irradiated with 2 MeV-electrons at a fluence of 1x1018/cm2 at RT. After irradiation, the samples were annealed between 600 and 1400oC in Ar. Photoluminescence (PL) measurements were carried out at RT to confirm NV creation. For PL measurements, the laser with a wavelength of 532 nm was used as excitation. PL intensity for samples annealed at 600 oC is about half even after annealing for 600 min, comparing with that for 800 oC-annealed samples although the values increase with increasing annealing time. Thus, the annealing at 650 oC is not enough to create NV. The samples annealed between 800 and 1200 oC show the highest PL intensity even after annealing for 10 min. The 800 and 1000 oC-annealed samples keep the PL intensity after annealing for 1200 min although the PL intensity for 1200 oC-annealed samples decrease with increasing annealing time above 100 min. The PL intensity for the samples annealed at 1400 oC shows smaller value and decreases with increasing annealing time. For T2, the samples annealed at 1400 oC show 2 microsec after annealing for 10 min. However, NV- cannot be observed after annealing at 1400 oC for 30min. Therefore, it can be concluded that annealing at 1400 oC is not suitable for the creation of NV-. For samples annealed between 600 and 1000 oC, the values of T2 are constant (between 0.5 and 0.9 microsec) after annealing up to 1200 min. For samples annealed at 1200 oC, no significant difference in T2 value is observed from those annealed between 600 and 1000 oC up to 30min, and the value increases with increasing annealing time above 30 min. From the point of view of sensing, it is important to consider both the amounts of NV- centers and T2. Therefore, we compare the values of PL intensity times T2. As a result, the samples annealed between 800 and 1200 oC show the highest value although the value for samples annealed at 1200 oC decreases after annealing for 1200 min. This suggests that annealing at 800 oC for 10 min is enough to create NV-s. We also study the creation of NV-s in diamonds by electron irradiation at elevated temperature. The samples with P1 concentration around 60 and 100 ppm were irradiated with 2 MeV-electrons at fluences up to 5x1018/cm2 at 800 or 1000 oC. The samples were annealed at 1000 oC for 120 min after irradiation. The amounts of NV are estimated from electron spin resonance (ESR) signals. As a result, samples irradiated at 800 and 1000 oC show higher NV- concentration than that for RT-irradiated ones, and 800 oC-irradiated ones show higher NV concentration than 1000oC-irradiated ones. Since the T2 values are not affected by irradiation temperature, the elevated temperature irradiation, especially 800 oC irradiation is a useful method to realize quantum sensing with high sensitivity.